Coating failure most likely starts here
After powder spraying or painting, local peeling, blistering, and early rust in the salt spray test often occur because the pre-treatment is not done properly. The surface of the die-casting part carries release agent, cutting fluid, aluminum chips and oxide scale. Any layer of residue will form a weak interface between the coating and the substrate. During the adhesion test, when the entire failed piece was peeled off, a shiny metal surface could often be seen on the cross section, indicating that the coating did not bite the substrate at all.
Three steps of degreasing, washing and transformation
Select the degreasing method according to the degree of oil pollution: for heavy oil pollution, use alkaline degreasing and ultrasonic waves, for light oil pollution, spray. The temperature and concentration are implemented according to the supplier's parameters, and the bath liquid is regularly tested and replaced. The bath liquid accumulated over time seems to be still usable, but the actual degreasing capacity has declined.
Washing should be graded. After degreasing, the first water wash takes over the bath liquid brought out, and the second clean water rinse. The water quality directly affects the results. Use deionized water for the final step, and control the conductivity below the set value. Direct rinsing with tap water will leave calcium and magnesium salts on the surface, which will form fine particles after spraying.
Aluminum parts are often treated with conversion coating. The film layer is thin and uniform, providing mechanical bite for the coating. The film is strictly controlled according to the process card. If it is too thick, it will be brittle, and it will easily peel off together with the coating during the impact test. Zinc alloy parts are sensitive to acidic media, and the pickling time should be short to avoid excessive corrosion and blackening of the surface. It is not advisable to leave the conversion film for a long time between completion and spraying. The film layer will absorb moisture and fail after the specified time, and needs to be reprocessed.
Drying and inspection
The pre-processed workpiece must be thoroughly dried. Water accumulation in ribs and screw holes is most easily ignored. If water is brought into the spray booth, the powder layer will not adhere well to the wet area and will form shrinkage holes after solidification. The drying temperature is set according to the material, and the die casting should not be too high to avoid deformation and surface oxidation.
- Use deionized water for final rinsing, and the conductivity is controlled according to the upper limit of the process card;
- Water film continuity check: if the water does not break continuously within 30 seconds after the water is discharged, it is qualified;
- The conversion film film is inspected according to the batch, and the pickling time is set individually according to the material;
- After drying, check the ribs and screw holes. If there is no water stain, transfer to the spray booth.
Weijiaxin’s surface treatment line lists tank liquid testing, rinsing water quality and drying temperature as shift record items. Batches that fail pre-treatment will not enter the spraying process. For the shell, the good-looking coating is only the first thing to look at. Whether it can last for several years outdoors, the answer lies in the pre-treatment tank.