Where do the pores come from?
Die casting presses molten metal into the mold cavity at high speed, and air entrainment is almost inevitable. There are three common sources: the gas involved in the filling process has no time to be discharged and remains in the last filled part; the thick wall cools slowly and the feeding is insufficient to form shrinkage holes; the exhaust channel is blocked or the exhaust position is improper, and the cavity gas has nowhere to go. The three types of defects have different shapes on the cross-section. The inner walls of the pores are relatively smooth and the shrinkage holes are irregular dendritic.
The pores themselves do not necessarily affect use. The tiny pores distributed in non-stressed and non-sealed areas have no substantial impact on the function of the shell as long as they are not connected to the surface; what really needs to be controlled are the pores that penetrate the wall thickness and the looseness below the sealing surface. To judge the degree of influence, we need to look at the relationship between the location of the pores and the direction of the wall thickness, rather than simply counting the number.
How does a pore turn into a leak?
The first is penetration. The pores are just connected to form a channel, leading from the inner cavity to the outer wall. Water vapor slowly penetrates under the pressure difference, which appears as a long-term slow leak rather than obvious dripping. It is difficult to detect in a short-term test. The second is post-processing exposure. There is a margin between the bottom surface of the sealing groove and the mating surface. After milling 0.4 mm, the pores originally buried under the skin are cut, forming surface pinholes that cannot be sealed even if the rubber ring is pressed up.
The third is the looseness under the sealing surface. Even if there is no opening on the surface, the pressure and screw pretightening force will act for a long time, and the loose area will gradually collapse, causing local depressions on the sealing surface. The compression amount of the rubber ring will be uneven along the circumference, and it will fail at the thinnest part first. This type of failure develops slowly and is not easy to detect in a short period of time. When troubleshooting, priority should be given to suspecting the density of the material below the sealing surface.
Judgment and improvement
Improvements on the process side start with the gate and exhaust: open the inner gate at a thick wall, so that the final filling position is near the exhaust groove; match the mold temperature with the injection speed to reduce cold shut and air entrainment; use local pressure or vacuum assistance for parts with high sealing requirements to increase the density of the area. The injection specific pressure and material temperature also need to match. Too high material temperature will aggravate air entrainment.
- Carry out X-ray inspection after the first mold and modified mold, focusing on the sealing surface and screw columns;
- Cut sections to observe whether there are exposed pores in the processing allowance layer;
- After processing the sealing surface, do fluorescence or color penetration to find pinholes;
- After the whole machine is assembled, keep it airtight and maintain pressure, and use pressure attenuation to locate the leaking area.
Weijiaxin listed pore distribution as a must-check item in the process review of sealed structural parts, and die casting and machining jointly confirmed the status of the remaining layer. The air hole cannot be completely eliminated, but it can be moved to a position where it does not affect the seal.