Effect of workshop temperature and humidity on shell coating

The first thing humidity affects is the powder itself

In August in South China, the relative humidity in the workshop is often above 80%. The first problem in the compressed air and powder conveying pipelines is the fluidity of the powder. The powder clumps when it gets wet, the spray gun output is intermittent, and the powder layer falling on the surface of the workpiece is uneven in thickness. Orange peel and particles will appear after solidification. When repairing such defects, the entire piece will need to be stripped of paint and repainted, and the cost is much higher than early moisture control.

The workshop method is to make the powder spraying room and the powder storage area into relatively independent spaces, and the dehumidifier is controlled by dew point rather than temperature. After the powder barrel is opened and used up on duty, the remaining powder should be sealed and stored to avoid repeated moisture absorption. The compressed air unit is equipped with a cold dryer and three-stage filtration, and the end of the pipeline is drained every shift. This is more direct than adjusting the temperature of the spray booth.

Temperature determines the leveling and curing of the paint film

When the temperature of the workpiece is lower than the ambient dew point, the powder layer will absorb moisture when sprayed on it, resulting in dense pinholes after curing. After pre-treatment and drying, the workpiece needs to be cooled to a temperature close to the spray booth before switching. The length of the cooling section is not enough. The workpiece enters the spray booth with residual temperature. The powder layer gels in advance at the corners, and the corner coverage decreases.

The setting of the baking curve should be modified according to the environment. In summer, the temperature of the workpiece entering the furnace is high. The heating section can be shortened, but the holding time cannot be shortened. Otherwise, the deep cavity position of the thick-walled die-casting part will not be cured enough and the whole piece will be easily peeled off during the adhesion test. The curing oven zone temperature measurement is calibrated once a quarter, and thermocouples are attached to the hanger and workpiece for comparison.

Write the environmental parameters into the inspection form

The environment is managed not by feeling but by recording. Weijiaxin fixed four items in the pre-shift inspection table of the coating line: temperature and humidity, dew point, compressed air pressure and filter pressure difference. If the set range is exceeded, the loading of parts will be stopped, and the environment will be adjusted first before starting the machine. This rule changes the environment from empirical judgment to traceable records, and the comparison of color batches also has a common premise.

  • The spray booth temperature is 20 to 28 degrees Celsius and the relative humidity is 50% to 70% as the conventional control range;
  • The workpiece temperature must be more than 3 degrees Celsius higher than the ambient dew point before loading the workpiece;
  • The compressed air pressure dew point is lower than minus 20 degrees Celsius, and the condensate water from the gas storage tank is discharged every shift;
  • The curing furnace conducts furnace temperature tracking every quarter and records the actual measured value of the deep cavity position.

For customers, these parameters are ultimately reflected in two things: no visible seams in the same batch of colors, and no blistering or chalking after one and a half years of outdoor use. Painting is not a separate process. It connects the workshop environment, pre-treatment and baking into a chain. If any link is loose, the appearance and weather resistance will deteriorate at the same time.

Back to list

Need a housing built for your camera?

Send us your drawings or samples — our engineering team will respond with a feasibility plan and quotation.