Inspection standards for die-cast alloy incoming materials are tightened again

Qualifying the composition does not mean that the batch is stable

When alloy ingots enter the factory, the traditional method is to check the grade and take a spectrum. If the main elements fall within the range, they are deemed qualified. The strength fluctuations and pinholes on the machined surface that occur during batch die casting are often not explained by the composition. The difference is hidden in the gas content, inclusions and recycled material ratio. Starting from September, Weijiaxin wrote these three items into the incoming material record and filed them together with the spectrum report.

The gas content cannot be measured accurately on solid ingots, but it can be judged from the fracture and surface: the fracture is dense and silver-white fine crystals, indicating that the degassing is in place during smelting; the fracture is dark with a black oxide film interlayer, and must be refined and degassed after being put into the furnace. Ingots with cold seals, shrinkage holes and obvious oxide scale on the surface should not be fed directly into the barrel.

Set a separate upper limit for the proportion of recycled materials

The recycled materials themselves are not the problem, the problem is that the proportion is out of control. Gates, cakes, and scrap parts are repeatedly returned to the furnace, and the iron content and gas content accumulate round by round, resulting in poor fluidity and insufficient filling of thin-walled parts. Stack the recycled materials separately according to their sources. Do not mix self-produced clean recycled materials with foreign scrap parts. The proportions should be written on the ingredient list. This is more effective than adjusting the injection parameters afterwards.

On-site judgment depends on two things: the amount of scum on the melt surface, and the filling status during continuous production of the same mold. If the scum increases significantly and undercasting begins to occur at the far end corner, it is time to go back and check the batching records instead of blindly increasing the mold temperature.

How to implement inspection items and judgment

There is no need to pursue too many items for incoming material inspection. The key is that each item can be judged and traced. The sampling position of each batch is fixed, and the composition, fracture, size and surface are recorded separately. Abnormal batches are individually identified and isolated, and are not mixed with other batches.

  • The main elements and impurity elements are spectrally checked batch by batch according to the brand, and the iron content is listed separately;
  • Take three samples from each batch to see the fracture surface, and record the density and inclusions;
  • Sampling inspection of the size and unit weight of the ingots to avoid material jamming and unstable feeding;
  • The proportion, source and batch number of the returned materials can be traced on the ingredient list.

After the standards are tightened, there is an additional procedure for procurement and workshops. In exchange, process parameters do not need to be adjusted frequently. For customers who make shells, this means that the wall thickness, strength and processing surface quality between different batches of the same part number are closer, and the conclusions from the trial mold and first piece confirmation can be continued to be used.

Back to list

Need a housing built for your camera?

Send us your drawings or samples — our engineering team will respond with a feasibility plan and quotation.